Touchstone Method for Testing Karat Gold Purity


There are a few scientific methods for precisely determining karat gold purity, some destructive (fire assay) and others nondestructive (X-ray florescence). Both methods require costly equipment, special procedures and a well-lit and ventilated area. A simpler method for determining gold purity in jewelry is the touchstone testing process, an age-old technique that is relatively nondestructive to jewelry and offers quick results.

3 Minute Read

HomeLearning CenterJewelry MakingBench Tips and TricksTouchstone Method for Testing Karat Gold Purity
By GIA Jewelry Arts InstructorsMore from this author
Updated on

There are a few scientific methods for precisely determining karat gold purity, some destructive (fire assay) and others nondestructive (X-ray florescence). Both methods require costly equipment, special procedures and a well-lit and ventilated area. A simpler method for determining gold purity in jewelry is the "touchstone" testing process, an age-old technique that is relatively nondestructive to jewelry and offers quick results.

Use with Care

Touchstone testing incorporates the use of acids, so close attention to safety and careful procedures are a must.

Touchstone testing is based on the fact that 24k gold resists all but the strongest acids. The purer the gold, the stronger the acid required to dissolve it. Measured strengths of nitric acid are used to test for 14k and lower. Aqua regia, a mixture of one part nitric acid and three parts hydrochloric acid, is used to test higher karat purity through the process of comparison and elimination.

To conduct touchstone testing, you'll need an acid testing kit (available through jewelry tool suppliers), a well-ventilated area, two glass beakers, water, baking soda, protective gloves, 320-grit abrasive paper, safety goggles and paper towels.

Your testing kit includes a set of testing needles. Each needle has a karat gold sample on its tip and the karat value stamped on the side. Use yellow gold needles for testing yellow gold and white gold needles for testing white gold.

Begin by checking the gold jewelry piece for other stampings (e.g., quality marks or manufacturer's marks) and make note of characteristics such as heft, color and reflectivity. If you suspect the item may not be gold, use an engraving tool and make a small notch in an unobtrusive place on the jewelry to expose fresh metal. Next, put on protective gloves and place a drop of acid from the 18k gold testing bottle over the small notch. A highly effervescent green reaction indicates base metal, and no further testing is required.

If there is little or no reaction, the piece is likely karat gold, and the next test is for purity. Follow these steps:

  • Rub the jewelry of unknown karat purity gently back and forth on the testing stone to leave a thin but clearly visible metal sample. Use care to take this sample from a place not clearly visible on the jewelry and away from solder joints.
  • With a testing needle, draw a question mark on the touchstone that represents the unknown metal.
  • Start with the 14-karat testing needle and rub a layer next to the unknown. Label it "14."
  • Repeat this process, making a layer and then labeling with the 18-, 22- and 10-karat testing needles.
  • Now choose the bottle labeled for testing 10-karat and lightly swipe the applicator across all the samples.
  • After approximately 20 to 40 seconds, place the touchstone in a mixture of baking soda and water to neutralize the acid in one beaker, then rinse in water in the other beaker.
  • Blot the touchstone with paper towels and observe. The 10-karat sample has dissolved, but the unknown metal is still visible. This confirms the unknown metal is finer than 10-karat.
  • Next, choose the bottle labeled for testing 14-karat and swipe it across the samples just below the first test.
  • Allow enough time for the acid to react and neutralize, then rinse and blot the touchstone and observe. The acid has dissolved both the 10- and 14-karat samples. The unknown metal is therefore 14-karat or slightly higher.

Always prepare the touchstone for its next use by cleaning it thoroughly. Remove the metal from the stone's surface by placing it facedown on a piece of 320-grit abrasive paper on a flat surface. Apply moderate pressure and sand it in a circular motion until sample layers are no longer visible. Neutralize, rinse and blot dry before replacing in the kit. Always follow the manufacturer's directions for the proper care, storage and handling of acids.

By GIA © 2011
In association with
Art Jewelry
For more information on GIA‘s Jewelry Manufacturing Arts program, click here.
All rights reserved internationally. Copyright © GIA. Users have permission to download the information and share it as long as no money is made-no commercial use of this information is allowed without permission in writing from GIA

You assume all responsibility and risk for the use of the safety resources available on or through this web page. The International Gem Society LLC does not assume any liability for the materials, information and opinions provided on, or available through, this web page. No advice or information provided by this website shall create any warranty. Reliance on such advice, information or the content of this web page is solely at your own risk, including without limitation any safety guidelines, resources or precautions, or any other information related to safety that may be available on or through this web page. The International Gem Society LLC disclaims any liability for injury, death or damages resulting from the use thereof.


GIA Jewelry Arts Instructors

The All-In-One Jewelry Making Solution At Your Fingertips

When you join the Ganoksin community, you get the tools you need to take your work to the next level.

Become a Member

Trusted Jewelry Making Information & Techniques

Sign up to receive the latest articles, techniques, and inspirations with our free newsletter.