Laser Welding Prong Repairs


1 Minute Read

By Steve SatowMore from this author
Updated on

This article provides a step by step procedure on how to do laser welding prong repairs on a ring.

Laser Welding Prong Repairs Project

image_1Use a separating disk to grind the prong flat. Place a redi-prong on a metal surface and tap gently to remove any flashing on bottom. Lay the redi-prong on the prong and check for tight fit.
image_2To tack redi-prong in place hold it with fine tweezers and shoot with a laser at the joint between the bottom of the redi-prong and the old prong.
image_3Side view ofprong tacked in place. Check to make sure the prong is tight against stone and tighten if necessary.
image_4Turn the ring around and shoot the laser down from the top to finish the seam between the new prong tip and the old prong.
image_5Place 30ga wire on welded joint and fill several passes with laser shooting from the side, until you achieve the original contour of the prong.
image_6Turn the ring until the top of the prong faces you. Shooting down toward the base of the prong with the laser, widen the beam and smear the metal down the back of the prong towards the base.

Continue this until the back of the prong is smooth.

image_7No pumice wheel should be needed to finish the back of the prong. I used a 6-inch knife edge wheel to concentrate the polishing on the prong only and then put it right into the cleaner.
image_8Finished product for new prongs took less then ten minutes from start to finish.
By Steve Satow – © Bench Magazine
In association with
BENCH Magazine is devoted to the Bench Jeweler in retail jewelry stores and small trade shops.
_______________________
Steve Satow is owner of Gem Services & Imaging and Senior Goldsmith at Saxon Jewelers & Engraving. Steve graduated from Bowman Technical School in Lancaster, PA in Aug. 1976, with additional GIA training in bench tricks, setting, wax, casting in place, and platinum, and received digital imaging training from GemVision Digital Goldsmith.

You assume all responsibility and risk for the use of the safety resources available on or through this web page. The International Gem Society LLC does not assume any liability for the materials, information and opinions provided on, or available through, this web page. No advice or information provided by this website shall create any warranty. Reliance on such advice, information or the content of this web page is solely at your own risk, including without limitation any safety guidelines, resources or precautions, or any other information related to safety that may be available on or through this web page. The International Gem Society LLC disclaims any liability for injury, death or damages resulting from the use thereof.


The All-In-One Jewelry Making Solution At Your Fingertips

When you join the Ganoksin community, you get the tools you need to take your work to the next level.

Become a Member

Trusted Jewelry Making Information & Techniques

Sign up to receive the latest articles, techniques, and inspirations with our free newsletter.