Intro to Enameling: Double-Sided Pendant 2


3 Minute Read

HomeLearning CenterJewelry MakingEnamelingIntro to Enameling: Double-Sided Pendant 2
By Woodrow W. CarpenterMore from this author
Updated on

For the last couple years The W.W. Carpenter Enamel Foundation has held "Intro To Enameling" workshops that are designed to walk beginning enamel students through multiple procedures in a short amount of time. Three projects were developed where choice of color and design considerations were minimized so that the focus is on enamel procedures.

The second project is a double sided pendant. (The first project was featured in the August '09 issue of Glass on Metal; the 3rd project will be featured in the February '10 issue).

making a double-sided pendant fig 1

What You Will Learn

  • Working on thin gauge copper (.0I0′ thick malleable copper)
  • Cutting copper with ordinary scissors
  • Removing oil or grease with Penny Brite
  • Coating both sides with enamel for the first firing
  • Using liquid brushable enamel
  • Dry brush stencil technique
  • Sgraffito (scratching through)
  • Stencil texture
  • Stencil blockout

Tools:

  • Scissors
  • Sifter
  • Toothpick
  • Brush
  • Postcard
  • Metal Stencil
  • Other Stencils
  • Pedestal
  • Phone Book Paper
  • Plastic Spoons
  • Toothbrush

Materials:

  • Penny Brite
  • LCE-1 Black
  • LCE-3 White
  • Opaque enamels:
    • 1870 Orient Red
    • 1685 Cobalt blue
    • 1820 Goldenrod Yellow
    • 1030 White
  • Glass of water
  • Malleable copper piece to be cut out with pre-drilled hole for jump ring.

Steps on Making a Double-Sided Pendant Project 2

image_2 (35)Cut out copper shape and drill holes (Fig. 1)
image_3 (33)Stone off any sharp points under water. Clean with Penny Brite and rinse thoroughly (Fig. 2)
image_4 (29)Fig. 3 Place LCE-1 Black (powder form) in plastic spoon and add enough water to make a milky solution. Apply with brush using a dabbing motion. Apply as evenly as possible. Dry.
image_5 (26)Fig.4 Turn piece over to opposite side. Apply 3 parts water, one part Klyr-fire with brush. Sift on coat of 1030 over wet Kyr-fire (Fig. 4). Clear holes of enamel with toothpick. Dry. Fire for 2 minutes at 1450 degrees F. Let cool. Stone edge to remove copper oxide.
image_6 (20)Fig. 5 Place LCE-3 White (powder form) in a plastic spoon and add enough water to make a thin milky solution, make it thinner than the black. Apply with a brush to the fired black side of the piece . Make sure it is not applied too thickly Better on the thin side than the thick side. Dry. DO NOT FIRE YET.
image_7 (15)image_8 (13)Take a metal stencil (available at scrapbook sections in craft supply stores, Fig. 6) or make your own stencil out of plastic with an exacto knife and place stencil onto unfired but dry, LCE-3 White (Fig.7).
image_9 (7)Fig 8 Hold without slipping and take a toothbrush and brush away dry LCE-3 White from openings in stencil.
image_10 (6)Fig. 9 Carefully lift up and blow away excess white.
image_11Fig. 10 With a sharpened wooden point like a toothpick, draw through the white for any additional crosshatches, borders, lines etc. that you would like to add to the stencil pattern. Blow away excess white.
image_11_1image_11_2Fig. 11 Turn piece over to other side and carefully place on pedestal. Take a postcard and slightly bend it so some of the postcard will lay on some part of the piece, acting as a block out material.

Use a 100 or 150 mesh sifter to apply either blue red, or yellow lightly over postcard and onto piece.

image_14 (5)image_15 (4)Fig. 12 Place the postcard in a different position and apply a light sifting of a second color (in this case yellow) over the unfired blue.
image_16 (4)image_17 (3)Fig. 13 Take another type stencil such as an embroiders mat and sift a contrasting color over the yellow. Sift very lightly as it is easy to over sift and lose detail.

This results in a textured pattern.

image_18 (3)Fig. 14 Take a metal or plastic stencil of an object, flower, bird etc, and sift again a contrasting color through the stencil and on top of the textured pattern. The finer 100 or 150 mesh screens will allow sharper enamel edges.
image_19 (3)Fig. 15 Carefully lift up stencil. Clear hole(s) of enamel with toothpick.
image_20 (3)Fig. 16 Pick up piece and place on trivet. Fire for 2 minutes at 450 degrees F. When cool, clean edges with medium jewelers file. Sand edges smooth with fine sand paper. Attach jump rings and cord and you have a pendant making use of many enamel procedures.
image_21 (3)Fig. 17 Variations of Project 2, front and back
Related Links:

Intro to Enameling Project 1 - Double-Sided Pendant
Intro to Enameling Project 3 - Cloisonne Pendant

Intro To Enameling Workshop
W.W. Carpenter Enamel Foundation
650 Colfax Ave., Building 2, Bellevue, KY 41073
Phone: 859-291-3800
Email: info@glass-on-metal.com
The W.W. Carpenter Enamel Foundation, the authors and instructors assume no liability for injury or harm to persons or property for any use of instructional or technical advice. All information is provided "as is" and is not warranted or guaranteed in any way.
Texts by Woodrow W. Carpenter and Tom ellis
Photos by Sandy Zureich
© Glass On Metal – Vol. 28, No. 5, December, 2009
In association
glass on metal
Glass on Metal is the only publication dedicated to enameling and related arts. Technical information, book reviews, how-to articles and insight on contemporary enamelers highlight each issue.

You assume all responsibility and risk for the use of the safety resources available on or through this web page. The International Gem Society LLC does not assume any liability for the materials, information and opinions provided on, or available through, this web page. No advice or information provided by this website shall create any warranty. Reliance on such advice, information or the content of this web page is solely at your own risk, including without limitation any safety guidelines, resources or precautions, or any other information related to safety that may be available on or through this web page. The International Gem Society LLC disclaims any liability for injury, death or damages resulting from the use thereof.


Woodrow W. Carpenter

The All-In-One Jewelry Making Solution At Your Fingertips

When you join the Ganoksin community, you get the tools you need to take your work to the next level.

Become a Member

Trusted Jewelry Making Information & Techniques

Sign up to receive the latest articles, techniques, and inspirations with our free newsletter.