Heatsensitive gemstones must no longer be removed from their setting when changing a ring size. This provides the goldsmith with immense time advantages. When joining the ring back together by welding instead of soldering the heat development is so low that the gemstone is not affected. The welding procedure is demonstrated using a simple ring made of 14 karat gold and the most practically tried and tested device PUK 2. www.lampert.info

Changing ring widths

Ring sizing: Exemplary wedding ring 14 karat yellow gold, 4mm x 2mm, half-round. 1_Fit the ring to the requested size and file until wedge shaped
2_Put similargold wire 0.4 to 0.5 mm into the joint, place the electrode next to the wire and melt on the material
3_Try to introduce the welding material in layers, even and tight
4_Fill up the joint until the introduced material juts out approx. 0.3 to 0.5 mm. Proceed in the same way on the back of the joint
5_The compactor has now been used to polish the joint
6_Apply high revolutions to bring the welded joint to the exact and requested height
7_The seam is trimmed or polished using a polisher or emery file
8_If the right strategy is used, the seam will be solid and without pores

by Christine Patrich

You assume all responsibility and risk for the use of the safety resources available on or through this web page. The International Gem Society LLC does not assume any liability for the materials, information and opinions provided on, or available through, this web page. No advice or information provided by this website shall create any warranty. Reliance on such advice, information or the content of this web page is solely at your own risk, including without limitation any safety guidelines, resources or precautions, or any other information related to safety that may be available on or through this web page. The International Gem Society LLC disclaims any liability for injury, death or damages resulting from the use thereof.


Christine Patrich

The All-In-One Jewelry Making Solution At Your Fingertips

When you join the Ganoksin community, you get the tools you need to take your work to the next level.

Become a Member

Trusted Jewelry Making Information & Techniques

Sign up to receive the latest articles, techniques, and inspirations with our free newsletter.